Material Properties
|
Test | Test method | Unit | Typical value |
Physicalpropertiesandmechanicalproperties |
|||
MeltFlowRate(21.6kg@150°C) |
AEIMethod |
g/10minutes |
15 |
Tensilestrength |
IEC60811-1-1 |
N/mm² |
14 |
Elongationatbreak |
IEC60811-1-1 |
% |
160 |
Density |
BS2782Pt.6Mtd620A-D |
g/cm3 |
1.47 |
Typicalageingbehaviourafter7daysat135°C |
|||
Tensilestrength |
IEC60811-1-2 |
%variation |
+5 |
Elongationatbreak |
IEC60811-1-2 |
%variation |
-10 |
Cureassessmentbyhotsettest(forced Elongationunderload(20N/cm2at200°C) |
curedat80°Cinwater) IEC60811-2-1 |
% |
30 |
Permanentelongationaftercooling |
IEC60811-2-1 |
% |
0 |
Thermomechanicalproperties |
|
|
|
HotPressureDeformation(100°C,K=1) |
IEC60811-3-1 |
% |
35 |
Fireandsmokeproperties |
|
|
|
Smokedensity |
ASTM2843:2004 |
% |
<3.5 |
Oxygenindex |
BSISO4589-2 |
% |
29 |
Temperatureindex |
BSISO4589-3 |
°C |
245 |
HalogenAcidgasevolution |
IEC60754-1 |
% |
<0.5 |
CorrosivityofGases |
IEC60754-2 |
pH |
4.6 |
Conductivityofgases |
IEC60754-2 |
µS/cm |
13 |
Electricalpropertiesat90°C |
|
|
|
Insulationresistance |
IEC60502 |
MΩ.km |
5 |
InsulationresistanceConstant(K)Volumeresistivity |
IEC60502 IEC60502 |
MΩ.kmOhm.cm |
1.5 4.4x1012 |
Extruder
Many modern thermoplastic extruders will process the material, although a screw designed to give good
homogenisation without excessive shear (which could cause unacceptable increases in melt temperature) should be
used. An extruder with an L/D ratio (length/diameter) of 15-24 and an extruder screw with a compression ratio 1.2:1
are recommended.
Extruder temperature conditions
It is important that the melt temperature is not allowed to increase above 160ºC. As a guide the following temperature
profile is recommended:-
Zone1 |
Zone2 |
Zone3 |
Zone4 |
Head |
Die |
130°C |
140°C |
145°C |
150°C |
160°C |
160°C |
This profile will vary slightly depending on extruder type, head design and output.
Screw water temperature - 40-60°C
Recommended screen pack: 50 (mesh apertures per linear inch) or 300 micron
Crosslinking or Cure
A satisfactory cure can be obtained either by immersion in hot water or exposure to low pressure steam at a
temperature up to 70°C. At the higher 10% addition levels of CM601 catalyst and under the correct conditions a
satisfactory cure is possible at ambient temperature and humidity.
Catalyst and Colour Masterbatches
CM601 catalyst masterbatch is normally added at between 5-10%.
Addition of approved colour masterbatches, including black, up to a maximum of 1%, has no detrimental effect on the
properties or crosslinking capability.
It is recommended that all masterbatches including those containing the catalyst should be thoroughly dried before
use for 8 hours at 60°C or 4 hours at 80°C in a de-humidifying drier.
Storage and Shelf Life
SX-0612 normally has shelf life of at least 6 months from the date of manufacture. The storage of silane crosslinkable
compounds in cool dry conditions will maximise useful shelf life. Other precautions are:-
• Packaging should remain sealed.
• Avoid temperature above 25°C.
• Avoid storage outside and in direct sunlight.
• Use within 8 hours of opening packaging.